Grades Of Alloy Steel Boiler Tubes

Oct 11, 2023

Grades of Alloy Steel Boiler Tubes

ASTM A335

ASTM A335 pipe for high-temperature operations is a smooth, ferritic alloy steel pipe. Pipe ordered in accordance with this specification is suitable for bending, vanstoning, and related forming and welding operations.

Chemical Composition Of ASTM A335

Grade

C

Mn

P Max

S Max

Si

Cr

Mo

Others

P5

0.15 Max

0.3-0.6

0.025

0.025

0.5 Max

4.00-6.00

0.45-0.65

 

P9

0.15 Max

0.30-0.60

0.025

0.025

0.25-1.00

8.00-10.00

0.9-1.1

 

P11

0.05-0.15

0.3-0.6

0.025

0.025

0.5-1

1-1.5

0.44-0.65

 

P12

0.05-0.15

0.3-0.61

0.025

0.025

0.5 Max

0.8-1.25

0.44-0.65

 

P22

0.05-0.15

0.3-0.6

0.025

0.025

0.5 Max

0.9-2.6

0.87-1.13

 

P36

0.1-0.17

0.8-1.2

0.03

0.025

0.25-0.5

0.3 Max

0.25-0.5

Ni:1.0-1.3,Cu 0.5-0.8,Nb 0.015-0.045,V 0.02Max,Al 0.05Max

P91

0.08-0.12

0.3-0.6

0.02

0.01

0.2-0.5

8-9.5

0.85-1.05

V 0.18-0.25,N 0.03-0.07,Ni 0.4Max,Al 0.02Max,Nb 0.06-0.1,Ti 0.01 Max,Zr 0.01Max

P92

0.07-0.13

0.3-0.6

0.02

0.01

0.5 Max

8.5-9.5

0.3-0.6

V 0.15-0.25,N 0.03-0.07,Ni 0.4max,Al 0.02max,Nb 0.04-0.09,W 1.5-2,B 0.001-0.006,Ti 0.01max,Zr 0.01max

EN 10216-2

These seamless steel pipes are intended for pressure applications. Steel, non-alloyed and alloy steel pipes with specified high-temperature properties.

Chemical Composition Of EN 10216-2 

Steel grade Steel
number
C Si Mn P
max
S
max
Cr Mo Ni
P235GH 1.0345 ≤ 0,16 ≤ 0,35 ≤ 1,20 0,025 0,020 ≤ 0,30 ≤ 0,08 ≤ 0,30

 

Al tot Cu Nb Ti max V Cr+Cu+Mo+Ni Others
≥ 0,020 ≤ 0,30 ≤ 0,010 0,040 ≤ 0,02 ≤ 0,70 -

Alloy Steel Boiler Tube

DIN 17175

DIN 17175 seamless boiler tubes are widely used in petroleum, boiler industry, thermal insulation, chemical fiber, chemical industry, medicine, machinery, paper making, mechanical equipment, refrigeration, food, energy, water conservancy, aerospace, transportation, aviation, marine, shipbuilding, environmental protection, boiler heat exchanger tubes.

Chemical composition of DIN 17175

Standard Grade Chemical Components (%)
C Si Mn P S Mo Cr
DIN17175 St 35.8 ≤0.17 0.10-0.35 0.40-0.80 ≤0.040 ≤0.040 / /
St 45.8 ≤0.17 0.10-0.35 0.40-0.80 ≤0.040 ≤0.040 / /
15Mo3 0.12-0.20 0.10-0.35 0.40-0.80 ≤0.035 ≤0.035 0.25-0.35 /
13CrMo44 0.10-0.18 0.10-0.35 0.40-0.70 ≤0.035 ≤0.035 0.45-0.65 0.70-1.10
10CrMo910 0.08-0.15 ≤0.50 0.40-0.70 ≤0.035 ≤0.035 0.90-1.20 2.0-2.50

JIS G3462

Usually used in heat exchangers, boilers, petroleum, chemical and other power fields, widely used because of high temperature resistance or corrosion resistance.

Chemical Composition of JIS G3462

JIS G3462 Grade C≤ Si≤ Mn≤ P≤ S≤ Cr Mo
STBA 12 0.10 ~0.20 0.10~0.50 0.30~0.80 0.035 0.035 - 0.45~0.65
STBA 13 0.15~0.25 0.10~0.50 0.30~0.80 0.035 0.035 - 0.45~0.65
STBA 20 0.10 ~0.20 0.10~0.50 0.30~0.60 0.035 0.035 0.050~0.080 0.45~0.65
STBA 22 0.15 0.50 0.30~0.60 0.035 0.035 0.80~1.25 0.45~0.65
STBA 23 0.15 0.50~1.00 0.30~0.60 0.030 0.030 1.00~1.50 0.45~0.65
STBA 24 0.15 0.50 0.30~0.60 0.030 0.030 1.90~2.60 0.87~1.13
STBA 25 0.15 0.50 0.30~0.60 0.030 0.030 4.00~6.00 0.45~0.65
STBA 26 0.15 0.25~1.00 0.30~0.60 0.030 0.030 8.00~10.00 0.90~1.10

Alloy Steel Boiler Tubes