Problems When Welding A335 P91
Feb 26, 2024
1. Generation of hardened structure in heat-affected zone
The critical cooling rate of P91 is low and the austenite stability is great. Normal pearlite transformation is not easy to occur during cooling, so martensite transformation occurs when cooling to a lower temperature. Because of this, P91 has a great tendency to harden and cold crack.
Since various tissues in the heat-affected zone have different densities, expansion coefficients and different lattice forms, they will inevitably be accompanied by different volume expansion and contraction during the heating and cooling processes; on the other hand, due to the uneven and Due to the high temperature, the internal stress of the P91 welded joint is very high.
For P91, austenite is very stable and needs to be cooled to a lower temperature (about 400°C) to change into martensite. The coarse martensite structure is brittle and hard, and the joints are under complex stress conditions. At the same time, during the cooling process of the weld, hydrogen diffuses from the weld to the near-seam area. The presence of hydrogen promotes martensite embrittlement. As a result of its combined effects, cold cracks are easily generated in the quenching zone.

2. Grain growth in heat affected zone
The welding thermal cycle has a significant impact on the grain growth in the heat-affected zone of the welding joint, especially the fusion zone adjacent to the highest heating temperature. When the cooling rate is small, coarse massive ferrite and carbide structures will appear in the welding heat-affected zone, which will significantly reduce the plasticity of the steel; when the cooling rate is large, due to the generation of coarse martensite structure, the plasticity of the steel will also be reduced. The plasticity of welded joints decreases.
3. Generation of softening layer
When P91 steel is welded in a quenched and tempered state, it is inevitable to produce a softening layer in the heat-affected zone, and the softening is more serious than that of pearlitic heat-resistant steel. When the heating and cooling speeds are slower, the degree of softening is greater. In addition, the width of the softened layer and its distance from the fusion line are not only related to the heating conditions and characteristics of the welding, but also related to preheating, post-weld heat treatment, etc.

4. Stress corrosion cracking
Before the post-weld heat treatment of P91 steel, the cooling temperature is generally not lower than 100°C. If it is cooled at room temperature and the environment is relatively humid, stress corrosion cracking will easily occur. German regulations: it must be cooled to below 150°C before post-weld heat treatment. When the workpiece is thick, has fillet welds, and has poor geometric dimensions, the cooling temperature should not be lower than 100°C. If it is cooled at room temperature, it is strictly prohibited to be wet, otherwise stress corrosion cracking will easily occur.