S31803 Stainless Steel Tube Production Specifications
Aug 19, 2024
1. Smelting and chemical composition of duplex steel
1.1 Smelting of duplex steel: smelting should be used electric furnace + vacuum refining or argon oxygen protection furnace;
1.2 Duplex steel chemical composition according to Table 1.
1.3 Requirements for ferrite in duplex steel in the phase proportion of: 40% - 50%. Percentage of ferrite content is determined according to ASTM E562.
Table 1
|
C ≤ |
Mn ≤ |
Si ≤ |
S ≤ |
P ≤ |
Cr |
Ni |
Mo |
Cu |
N |
|
0.030 |
2.0 |
1.0 |
0.020 |
0.030 |
22.0-23.0 |
4.50-6.50 |
3.0-3.50 |
0.3 |
0.14-0.20 |
1.4 on the billet should be equivalent to the head of the ingot to take samples, according to ASTM E381 by acid immersion low times the test shall not be visible to the naked eye, white spots, shrinkage, bubbles, cracks, inclusions, flap and delamination, and other defects; allow the existence of the general laxity, central laxity, segregation of not more than 1.5 levels of low times the organization of the defects.
1.5 Inclusions test on round steel specimens, according to ASTM E45 assessment of inclusions in steel.
Table 2
| Sulfide Class A | ≤1.0 | Silicate C | ≤1.5 | A+B+C+D |
| Aluminate B | ≤1.5 | Oxide D | ≤1.0 | ≤4 class |
2. Mechanical properties requirements: (according to ASTM A370 mechanical properties of steel products test methods and definitions for testing)
Table 3
| Tensile strength (MPa) ≥ | Yield strength (MPa) ≥ |
Elongation (%) ≥ |
Hardness ≤ | |
| Brinell HB | Rockwell HRC | |||
| 620 | 450 | 25 | 290 | 30.5 |
Hardness test is to measure the material heat treatment of an important indicator, each batch of test specimens not less than 2 pieces, each piece of three points, the value of each point should be in line with the requirements of Table 3.
3. Geometric deviation
| Specification | Allowable deviation (mm) |
Bend mm/m |
|||
| Outer diameter | Wall thickness | Length | |||
| Φ25×2×8901 | ±0.2 | ±12% | +6 | -0 | 1.5 |
Stainless Steel Pipe


4. Corrosion test
4.1 Specimens should be in accordance with ASTM A 262 E method of intergranular corrosion test
4.2 According to the provisions of the ASTM G48 standard, in 10% FeCl3 solution for pitting corrosion test 40 ℃ no pitting corrosion is qualified.
5. Non-destructive testing
5.1 According to the provisions of ASTM E426 standard for seamless steel pipe electromagnetic (eddy current) test.
5.2 According to the standard of the enterprise to do seamless pipe 100% underwater air pressure test.
6. Process performance test
Flattening test and flaring test according to ASTM A450 standard.
7.Inner and outer surface
The internal and external surfaces of the finished pipe shall be inspected according to the requirements of ASTM A790.
8.Delivery status
Solid solution heat treatment, pickling state delivery.
9.Packing
The cross-section is six-sided diamond shape for bundling, woven bag package. Attached with the name of the manufacturer, product name, specifications, quantity and weight, ordering unit and contract number, factory number and date of the certificate of conformity.
10. Quality certification documents
Should contain the following content:
a. Chemical composition (melting analysis, finished product analysis)
b. Ferrite content of the finished pipe determination of the value.
c. Mechanical properties test values and hardness values.
d. Acid dip low times test report
e. Heat treatment temperature, holding time, cooling method,
f. Corrosion test conclusion
g. Process performance test data
h. Conclusion and data of non-destructive testing
11. Additional requirements
In addition to meeting the above basic requirements, the following conditions must also be met:
a. The point sensitivity factor PREN is not less than 33 where PREN is calculated by the following formula:
PREN=%Cr+3.3*%Mo+16*%N
Therefore it must be ensured that: Cr(21.8 ~ 23) ; Mo(2.8 ~ 3.5) N( 0.13 ~ 0.2)
b. Ferrite and austenite are evenly distributed accordingly, with no precipitated third phase.
c.Design service life of 20 years