A199 T22 Seamless Tube: 2.25Cr-1Mo Heat Exchanger Tube Data
Jul 14, 2023
What A199 T22 Tube Is
ASTM A199 T22 is a seamless cold-drawn intermediate alloy-steel tube for heat exchangers and condensers. Although the grade is often loosely described as carbon steel tube, T22 is a ferritic 2.25Cr-1Mo low-alloy steel (UNS K21590), not a plain carbon grade: the chromium and molybdenum additions are what give the material its resistance to oxidation and to hydrogen attack at elevated temperature. The same analysis appears in three product forms, and the choice between them depends on service temperature, required heat treatment and test regime: A199 T22 cold-drawn tube, A213 T22 boiler, superheater and heat-exchanger tube, and A335 P22 seamless high-temperature pipe.
Chemical Composition and Mechanical Properties
| Element | Requirement (%) |
|---|---|
| Carbon (C) | 0.05–0.15 |
| Manganese (Mn) | 0.30–0.60 |
| Phosphorus (P), max | 0.025 |
| Sulfur (S), max | 0.025 |
| Silicon (Si), max | 0.50 |
| Chromium (Cr) | 1.90–2.60 |
| Molybdenum (Mo) | 0.87–1.13 |
| Property | Requirement, cold-drawn tube |
|---|---|
| Tensile strength Rm | 415 MPa minimum |
| Yield strength ReL | 205 MPa minimum |
| Elongation A | 30 % minimum |
| Hardness | 85 HRB (163 HBW) maximum |
Because the chromium and molybdenum content is what carries the elevated-temperature performance, grade verification by heat analysis, and by positive material identification on finished tubes, is normal practice on this grade. A tube that is dimensionally correct but carries the wrong Cr or Mo level will not perform in service.
Heat Treatment and Product Forms
Cold-drawn A199 tube is normally supplied annealed or isothermally annealed, which is what the intermediate classification of this specification implies: the tube is intended for fabrication and further assembly rather than for the most severe pressure part duty. Where the tube has to operate at elevated temperature, the equivalent A213 T22 grade is specified instead, supplied normalised and tempered at a controlled minimum temperature so that the microstructure is stable in service, with defined hardness limits and test frequency. For large-bore lines the matching pipe grade is used.
| Standard and form | Designation |
|---|---|
| ASTM A199, cold-drawn heat exchanger and condenser tube | T22 (UNS K21590) |
| ASTM A213, boiler, superheater and heat exchanger tube | T22 |
| ASTM A335, seamless pipe for high-temperature service | P22 |
| EN 10216-2, seamless steel tubes for pressure purposes | 10CrMo9-10 (1.7380) |
Size Range, Testing and Inspection
Typical supply range covers outside diameter 10–1000 mm, wall thickness 1–80 mm and length 1–12 m, with the exact dimensional tolerances taken from the standard selected.
Surface treatment is black paint or varnish, anti-corrosion oil, galvanising, or another treatment agreed at order stage.
Pipe ends are protected with plastic caps. Tubes and pipes are labelled and bundled with steel strip for shipment, or delivered loose in containers.
Each batch is supplied with a mill test certificate giving heat analysis, tensile, yield, elongation and hardness results, together with flattening, flaring and either hydrostatic or eddy-current test records as required.
Where the end use demands it, third-party inspection and positive material identification can be arranged to the purchase specification.
Applications of 2.25Cr-1Mo Tube and Pipe
Heat exchanger and condenser tubing in refinery, petrochemical and power plant service where the duty temperature is beyond the range of plain carbon steel.
Boiler and superheater tubes and steam piping at moderate steam temperatures, supplied as A213 T22 and A335 P22 respectively.
Hydroprocessing and other hydrogen-containing services, where the Cr-Mo chemistry gives the resistance to hydrogen attack that a carbon steel would lack; the allowable conditions are set by the applicable design code.
Furnace, transfer line and general high-temperature process piping, and internal components such as header stubs and supports.
FAQ
Q: Is A199 T22 a carbon steel?
No. It is a 2.25Cr-1Mo ferritic low-alloy steel, UNS K21590. It is sometimes listed with carbon steel grades because it is not stainless and contains only about 2.25 % chromium, but the alloying additions control its high-temperature behaviour.
Q: What is the difference between A199 T22 and A213 T22?
A199 covers cold-drawn intermediate alloy-steel heat exchanger and condenser tube, normally supplied annealed, while A213 covers boiler, superheater and heat exchanger tube supplied normalised and tempered with defined hardness limits and test frequency. For elevated-temperature pressure parts, A213 T22 is the usual choice.
Q: What are the equivalent grades?
A213 T22 tube and A335 P22 pipe share the same 2.25Cr-1Mo analysis, UNS K21590. The closest European designation is EN 10216-2 grade 10CrMo9-10, material number 1.7380.
Q: What temperature range is this grade used in?
As general guidance, 2.25Cr-1Mo is selected for metal temperatures up to roughly 580 °C; above that the creep strength falls away quickly and higher-chromium grades take over. The governing design code, not a general figure, decides the allowable stress for a specific project.
Q: How is quality verified on delivery?
The mill test certificate carries heat analysis, tensile, yield, elongation and hardness results plus flattening, flaring and hydrostatic or eddy-current records. Positive material identification is commonly requested to confirm the Cr and Mo content on finished tubes.