ASTM A213 for alloy and stainless steel tube
Nov 04, 2025
This standard applies to seamless ferritic and austenitic boiler, superheater, and heat-exchanger tubes, with specified grade designations such as T5, TP304, etc., as listed in Tables 1 and 2.
The requirements for grade designations that include the suffix 'H' differ from those of the corresponding grade without the 'H' suffix. These additional requirements provide these grades with superior creep-rupture strength compared to the corresponding grades without these requirements.
The tubes supplied under this standard are typically available in sizes and thicknesses ranging from 1/8 in (3.2 mm) inside diameter to 5 in (127 mm) outside diameter, with minimum wall thickness (or average wall thickness, if otherwise specified in the purchase order) from 0.015 to 0.500 in (0.4–12.7 mm). Other sizes may be provided, provided that all other requirements of this standard are met.
Values stated in inch-pound or SI (International System of Units) units are to be regarded as standard. The SI units are shown in parentheses in this standard. Since the values in the two unit systems are not exactly equivalent, each system must be used independently. Mixing the two unit systems will result in non-compliance with this standard. Unless the "M" (SI unit) designation is specified in the purchase order, the inch-pound unit system shall apply.
Specification
Standard: ASTM A213 for alloy and stainless steel tube
Grade: T2 T5 T9, T11, T22, T91, T92, TP304/L, TP316/L, TP317/L, TP321/H etc
OD: 1/8" to 16". 3.2mm to 406mm
WT: 0.015" to 0.500", 0.4mm to 12.7mm
Length: 10ft, 20ft, 40ft, or customized length
ASTM A213 Alloy Tube Chemical Composition
| Grade | UNS Designation | C | Mn | P | S | Si |
| A213 T2 | K11547 | 0.10–0.20 | 0.30–0.61 | 0.025 | 0.025B | 0.10–0.30 |
| A213 T5 | K41545 | 0.15 | 0.30–0.60 | 0.025 | 0.025 | 0.5 |
| A213 T5b | K51545 | 0.15 | 0.30–0.60 | 0.025 | 0.025 | 1.00–2.00 |
| A213 T5c | K41245 | 0.12 | 0.30–0.60 | 0.025 | 0.025 | 0.5 |
| A213 T9 | K90941 | 0.15 | 0.30–0.60 | 0.025 | 0.025 | 0.25–1.00 |
| A213 T11 | K11597 | 0.05–0.15 | 0.30–0.60 | 0.025 | 0.025 | 0.50–1.00 |
| A213 T12 | K11562 | 0.05–0.15 | 0.30–0.61 | 0.025 | 0.025B | 0.5 |
| A213 T17 | K12047 | 0.15–0.25 | 0.30–0.61 | 0.025 | 0.025 | 0.15–0.35 |
| A213 T21 | K31545 | 0.05–0.15 | 0.30–0.60 | 0.025 | 0.025 | 0.50–1.00 |
| A213 T22 | K21590 | 0.05–0.15 | 0.30–0.60 | 0.025 | 0.025 | 0.5 |
| A213 T23 | K40712 | 0.04–0.10 | 0.10–0.60 | 0.03 | 0.01 | 0.5 |
| A213 T24 | K30736 | 0.05–0.10 | 0.30–0.70 | 0.02 | 0.01 | 0.15–0.45 |
| A213 T36 | K21001 | 0.10–0.17 | 0.80–1.20 | 0.03 | 0.025 | 0.25–0.50 |
| A213 T91 | K90901 | 0.07–0.14 | 0.30–0.60 | 0.02 | 0.01 | 0.20–0.50 |
| A213 T92 | K92460 | 0.07–0.13 | 0.30–0.60 | 0.02 | 0.01 | 0.5 |
Mechanical properties of ASTM A213 alloy steel pipes
|
Steel Grade
|
Mechanical Properties |
|||
|
T. S |
Y. P |
Elongation |
Hardness |
|
|
T5 |
≥ 415MPa |
≥ 205MPa |
≥ 30% |
163HBW(85HRB) |
|
T9 |
≥ 415MPa |
≥ 205MPa |
≥ 30% |
179HBW(89HRB) |
|
T11 |
≥ 415MPa |
≥ 205MPa |
≥ 30% |
163HBW(85HRB) |
|
T12 |
≥ 415MPa |
≥ 220MPa |
≥ 30% |
163HBW(85HRB) |
|
T22 |
≥ 415MPa |
≥ 205MPa |
≥ 30% |
163HBW(85HRB) |
|
T91 |
≥ 585MPa |
≥ 415MPa |
≥ 20% |
250HBW(25HRB) |
Heat Treatment Procedures for ASTM A213 Alloy Tube
a. For grades T9, T11, T22, heat treatment methods are full or isothermal anneal, normalize and temper. (For conditions in later option, tempering temperature for T9 and T22 is above 675℃, T11 is above 650℃.)
b. For grades T91, T92, shall be normalize and temper, where normalizing shall be above 1040℃, tempering shall be above 730℃. As the delivery conditions.
Manufacturing Process of ASTM A213 Seamless Steel Pipes
Piercing: A preheated solid round billet (typically rolled or forged to ensure quality) is pierced in a piercing mill to form a hollow shell.
Hot Rolling: The pierced shell is rolled through multiple passes on a pipe rolling mill to reduce the outer diameter and wall thickness while improving the microstructure. Common equipment includes automatic rolling mills or periodic rolling mills.
Cold Rolling: For pipes requiring higher dimensional accuracy, better surface finish, or thinner wall thickness, the hot-rolled pipe undergoes further cold rolling. Cold rolling is performed at room temperature, significantly improving dimensional precision and surface smoothness.
Cold Drawing: Similar to cold rolling, this process is also conducted at room temperature, where the pipe is pulled through a die to further reduce dimensions and enhance precision and surface quality.
ASME A213 alloy seamless tube outer diameter tolerances
|
Hot rolled |
Outside Diameter, mm |
Tolerance, mm |
|
OD≤101.6 |
+0.4/-0.8 |
|
|
101.6<OD≤190.5 |
+0.4/-1.2 |
|
|
190.5<OD≤228.6 |
+0.4/-1.6 |
|
|
Cold Drawn |
Outside Diameter, mm |
Tolerance, mm |
|
OD<25.4 |
±0.10 |
|
|
25.4≤OD≤38.1 |
±0.15 |
|
|
38.1<OD<50.8 |
±0.20 |
|
|
50.8≤OD<63.5 |
±0.25 |
|
|
63.5≤OD<76.2 |
±0.30 |
|
|
76.2≤OD≤101.6 |
±0.38 |
|
|
101.6<OD≤190.5 |
±0.38/-0.64 |
|
|
190.5<OD≤228.6 |
±0.38/-1.14 |
Test and inspection

Packaging and shipping