Measures to prevent A335 P22 welding cracks

Feb 27, 2024

1. The welding rod must be dried strictly according to the requirements before use and stored in an insulating cylinder to maintain a certain temperature. It can be taken as needed. The welding rod must not be exposed to the air.
2. The thickness of the TiG welding base layer shall not exceed 5mm, but shall not be less than 3mm. For welding parts with high rigidity, in order to avoid breakdown of the root bead, the TiG welding process of 2 layers is used, and the thickness of the 2 layers does not exceed 6mm. When the temperature drops below about 10°C, in order to prevent primer cracks, preheat to about 100°C before TiG welding primer.

SA335 P22 Welding Tube

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 


3. Cancel the first layer of filling in SMAW welding before preheating. Preheat to 250-350℃ and the temperature on both sides of the welding joint is uniform before performing SMAW filling welding.
4. Keep the interlayer temperature not lower than 250℃ and not higher than 400℃.
5. For pipes with a wall thickness greater than or equal to 70mm, slow cooling measures should be taken when welding is interrupted.

alloy welding pipe

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 


6. Adopt a reasonable welding sequence. When SMAW welding, the two people always maintain symmetrical welding.
7. Strictly abide by the thin layer welding process and select appropriate welding specifications.