A213 T22 Boiler Tube: 2.25Cr-1Mo Alloy Steel Properties and Uses

Mar 05, 2025

A213 T22 is a seamless ferritic alloy steel tube made from a 2.25% chromium and 1% molybdenum composition. It is standardised in ASTM A213 and its ASME counterpart SA213, which cover seamless ferritic and austenitic alloy steel boiler, superheater and heat exchanger tubes. The combination of chromium and molybdenum gives the tube a creep strength that plain carbon steel cannot match, which is why T22 remains one of the most widely ordered alloy tube grades in refinery and power plant work.

What ASTM A213 T22 Covers

The A213 specification sets chemical composition, tensile requirements, hardness limits, heat treatment and testing for seamless alloy tube. T22 sits in the middle of the chromium range of the specification: it is stronger at temperature than the 1.25Cr grades, and considerably cheaper and easier to weld than the 9Cr martensitic grades. Tubes are used as superheater and reheater elements, heat exchanger bundles, furnace and convection tubes, and general high temperature transfer lines.

Standard: ASTM A213 / ASME SA213, seamless ferritic and austenitic alloy steel tube for boiler, superheater and heat exchanger service

Alloy class: 2.25Cr-1Mo low alloy steel

Equivalent product forms: A335 P22 for pipe, A182 F22 for forgings, A387 Gr.22 for pressure vessel plate

Typical size range: outside diameter 6 mm to 168 mm, wall thickness 1 mm to 25 mm

Delivery condition: heat treated (normalized and tempered), with hardness and tensile results on the certificate

Chemical Composition of A213 T22

Element Minimum, % Maximum, % Function
C 0.05 0.15 Strength and hardenability
Si - 0.50 Deoxidation, oxidation resistance
Mn 0.30 0.60 Toughness and hot workability
P - 0.025 Impurity control, weldability
S - 0.025 Limits hot shortness
Cr 1.90 2.60 Oxidation and corrosion resistance
Mo 0.87 1.13 Creep strength at elevated temperature

The chromium content forms a protective oxide layer that slows steam oxidation up to the design limit of the grade, while molybdenum strengthens the carbide network and delays creep deformation. Manganese is specified from 0.30% upward because it contributes to toughness and to the response of the steel during hot rolling.

Mechanical Properties

Property Requirement Notes
Tensile strength Rm 415 MPa min Room temperature test on the finished tube
Yield strength Rp0.2 205 MPa min Design basis for internal pressure calculations
Elongation A 30% min Confirms ductility for bending and swaging
Hardness 163 HBW max Controls the tempered condition and machining behaviour

Because the service condition is high temperature, the room temperature values above are only the acceptance floor. Design work uses the elevated temperature yield and creep rupture data for 2.25Cr-1Mo steel, where the allowable stress falls steadily as the metal temperature rises toward the upper limit of the grade.

Heat Treatment and Delivery Condition

T22 tube is delivered in the heat treated condition. Mill practice for 2.25Cr-1Mo tube normalizes in the region of 900-960 C and then tempers above roughly 675 C, producing a ferrite and tempered bainite structure with uniform hardness through the wall. The exact cycle is recorded on the inspection certificate, because the tempering temperature strongly influences both the hardness result and the impact toughness of the finished tube. Tubes that have been cold drawn are heat treated after the final drawing pass so that the specified mechanical properties apply to the delivered product and not to an intermediate stage.

Fabrication, Applications and Equivalent Grades

Welding is carried out with matching 2.25Cr-1Mo consumables, preheat, controlled interpass temperature and post-weld heat treatment. Bending and swaging are common because the tube is used in densely packed superheater banks, and the specified elongation of 30% gives the ductility required for those operations.

Superheater, reheater and economiser tube elements in power boilers

Heat exchanger and convection tube bundles in refineries and chemical plants

Reactor and furnace internals exposed to high temperature process gas

High temperature transfer lines and thick wall steam pipe in the A335 P22 product form

High temperature hardware in aerospace test and engine support systems

When a project is designed to an American code, T22 tube can be combined with P22 pipe and F22 forgings from the same alloy class, which keeps welding procedures, filler metal and post-weld heat treatment practice consistent across the whole pressure envelope. Substitution by a 1.25Cr grade is only acceptable after the allowable stress at design temperature has been rechecked, because the creep strength of 2.25Cr-1Mo is substantially higher in the 500-580 C band.

Frequently Asked Questions

Q: What is the chemical composition of A213 T22?
T22 contains 0.05-0.15% carbon, up to 0.50% silicon, 0.30-0.60% manganese, 1.90-2.60% chromium and 0.87-1.13% molybdenum, with phosphorus and sulphur each limited to 0.025% maximum.

Q: What are the mechanical requirements for T22 tube?
The finished tube must reach a minimum tensile strength of 415 MPa, a minimum yield strength of 205 MPa, at least 30% elongation and a maximum hardness of 163 HBW.

Q: Is A213 T22 the same as A335 P22?
They belong to the same 2.25Cr-1Mo alloy class but are different product forms: A213 T22 is seamless tube for boiler and heat exchanger service, while A335 P22 is seamless pipe for high temperature piping systems. They are frequently used together in one unit.

Q: What temperature can T22 tube be used at?
It is applied in the intermediate temperature band between the 1.25Cr grades and the 9Cr grades, typically up to about 580 C, and the governing limit for a specific component is the allowable stress at the design metal temperature.

Q: How is the tube supplied?
It is supplied in the normalized and tempered condition, produced by cold drawing, hot rolling or hot expanding, with tensile, hardness and flattening tests and the heat number recorded on the inspection certificate.

Q: Does T22 tube need post-weld heat treatment?
Yes for production welds. The joint is welded with preheat and matching filler metal, then post-weld heat treated below the original tempering temperature to relieve residual stress without softening the parent tube.