Welded API 5L X42 Steel Pipe
Coating: FBE, 3LPE, 3LPP, coal tar epoxy, black varnish, internal flow coating
Testing: Hydrostatic every joint; seam NDT (mandatory PSL2, on request PSL1); flattening on ERW; weld tensile; CVN on PSL2
Documentation: EN 10204 3.1; 3.2 where third-party witnessing is specified
Gnee Steel (Tianjin) Co., Ltd. is one of the most reliable manufacturers and suppliers of welded api 5l x42 steel pipe in China, also supports customized service with low price. Welcome to wholesale discount welded api 5l x42 steel pipe for sale here from our factory. Contact us for free sample.
API 5L X42 is L290 in ISO 3183, and GB/T 9711 uses the same number. The 42 is thousands of pounds per square inch of minimum yield: 42,100 psi, or 290 MPa. The minimum tensile is 415 MPa, which is exactly the same figure as Grade B. The two grades differ only in yield, and that one difference is worth about 15% of the steel in a pressure-controlled wall.
Welded X42 line pipe is made three ways. ERW and HFW pipe is formed from slit coil through a series of rolls and welded along one longitudinal seam at 100–400 kHz, then seam-normalised in line; it covers 21.3 mm to 609.6 mm outside diameter. LSAW pipe is formed from plate on a JCOE or UOE press, welded inside and out with submerged arc, then cold expanded; it covers roughly 406 mm to 1524 mm. SSAW pipe is wound from coil at a helix angle and welded on both sides of the spiral; it reaches 2540 mm and beyond. All three are supplied in PSL1 or PSL2, in random lengths of 5–7 m or 11–13 m or cut to a lay schedule, with plain, bevelled or threaded ends, FBE, 3LPE, 3LPP or black varnish coating, hydrostatically tested joint by joint, and released against an EN 10204 3.1 certificate, with 3.2 where a third party witnesses the tests.
Specification
| Item | Specification |
|---|---|
| Standard | API 5L 45th/46th edition, harmonised with ISO 3183; GB/T 9711 equivalent |
| Grade | X42 / L290 |
| Product specification level | PSL1 or PSL2 - both are available at this grade |
| Pipe type | Type E (electric welded), Type W (welded with filler metal), Type S (seamless, for comparison) |
| Welding routes | ERW / HFW; LSAW (JCOE, UOE); SSAW / HSAW |
| Outside diameter | ERW 21.3–609.6 mm (1/2–24 in); LSAW 406–1524 mm; SSAW 406–2540 mm and above |
| Wall thickness | ERW 2.0–20 mm typical; LSAW 6–50 mm; SSAW 5–25.4 mm from coil |
| Length | SRL 5–7 m, DRL 11–13 m, 6 m and 12 m fixed, up to 18 m on LSAW |
| Pipe ends | Plain, bevelled 30° with 1.6 mm root face, or threaded and coupled |
| Coating | FBE, 3LPE, 3LPP, coal tar epoxy, black varnish, internal flow coating |
| Testing | Hydrostatic every joint; seam NDT (mandatory PSL2, on request PSL1); flattening on ERW; weld tensile; CVN on PSL2 |
| Documentation | EN 10204 3.1; 3.2 where third-party witnessing is specified |
Chemistry from Table 6 and properties from Table 7 of API 5L; Charpy from Table 9. Element limits for PSL2 are maximums, and the carbon equivalent is a separate ceiling that the element limits do not guarantee - see section 4. Confirm all values against the edition named on the order.
What "Welded" Adds to an X42 Order
Two pipe orders can both read "API 5L X42, 12 inch, SCH 20" and still describe different products, because welding introduces four variables that seamless pipe does not have. The welding process, the position of the seam, the heat treatment applied to that seam, and the inspection coverage over it. All four are in the standard. None of them is implied by the grade.
API 5L handles the first of these with a type letter. Type S is seamless. Type E is electric welded, which covers ERW, LFW and HFW - one longitudinal seam, no filler metal, the weld made by resistance. Type W is welded with filler metal, which covers SAWL, SAWH and COW. Type F is continuous welded, and the standard restricts it to Grade A25, so it will not appear on an X42 order. A purchase order that omits the type letter has left the mill free to choose, and the mill will choose whatever its line is set up for that week.
The position of the seam matters more than it looks. A longitudinal seam runs parallel to the pipe axis, so it crosses every girth weld at 90°, and the two welds meet as a cross. A helical seam approaches the girth weld at an acute angle and the intersection becomes a long, shallow T. Radiography reads the first of those far more easily than the second, which is one of the quieter reasons helical pipe is priced lower at large diameter. It is not a quality difference in the pipe itself; it is a difference in how easily the joint can be proved.
For X42 specifically, the practical consequence is this. At 4 inch and below, ERW dominates and the seam question is settled by the mill's coil source. From 16 inch upward, LSAW and SSAW enter, and the seam question becomes a commercial one worth asking. Between 12 and 20 inch, all three routes can quote, and that overlap is where most of the price spread on an X42 enquiry comes from.
Three Routes, and the Sizes Each One Owns
The three welding routes are not competing for the same work. Each has a diameter band where it is the natural choice, and the bands overlap only at the edges.
| Route | Seam | Forming | OD range | Wall | Where it wins |
|---|---|---|---|---|---|
| ERW / HFW | One longitudinal, resistance welded, no filler | Coil slit, edge-trimmed, roll formed | 21.3–609.6 mm | 2.0–20 mm | Distribution mains, services, small-diameter gathering; lowest cost per tonne below 16 in |
| LSAW (JCOE / UOE) | One longitudinal, submerged arc, inside and out | Plate crimped, J or U pressed, O formed, cold expanded | 406–1524 mm | 6–50 mm | Heavy wall at large diameter; sizes where coil cannot reach the wall |
| SSAW / HSAW | One helical, submerged arc, inside and out | Coil wound at a fixed helix angle | 406–2540 mm and above | 5–25.4 mm | Large diameter at moderate wall; cheapest route where the D/t ratio is high |
The economics behind that table are simple once the seam is counted. An ERW mill buys coil by the tonne and sells pipe by the tonne, and the only material it wastes is the edge trim. An LSAW mill buys plate, which costs more per tonne than coil, and it has to crimp and press every shell before a single arc is struck. A spiral mill buys coil again, but it lays down two to three times as much weld per metre of pipe as a longitudinal mill, because the seam runs around the barrel rather than along it.
At 24 inch and 12.7 mm wall, all three routes can make the pipe. ERW will be cheapest if the mill can reach that wall on that diameter, which most cannot. LSAW will be the most expensive per tonne and the most dimensionally accurate. Spiral will sit between them and will be the only one of the three that can go to 48 inch without changing anything except the helix angle.
Chemistry: Two Numbers Decide the Heat
PSL1 and PSL2 do not differ much at X42 in the way most summaries suggest. The element limits move a little. What changes is that PSL2 adds a carbon equivalent ceiling, and that ceiling - not the carbon limit - is what constrains the steel.
PSL1
| Element, % max | Seamless | Welded |
|---|---|---|
| C | 0.28 | 0.26 |
| Mn | 1.30 | 1.30 |
| P | 0.030 | 0.030 |
| S | 0.030 | 0.030 |
| Nb + V + Ti | 0.15 combined | 0.15 combined |
| Cu / Ni / Cr / Mo | 0.50 / 0.50 / 0.50 / 0.15 | 0.50 / 0.50 / 0.50 / 0.15 |
| Carbon equivalent | No limit, and no requirement to report it | |
Manganese may rise by 0.05% for every 0.01% that carbon falls below its maximum, to a cap of 1.65% for grades up to X52. Copper, nickel and chromium may not be deliberately added at PSL1; the limits exist to cap what arrives in the scrap.
PSL2
| Element, % max | X42R | X42N | X42Q | X42M |
|---|---|---|---|---|
| C | 0.24 | 0.24 | 0.18 | 0.22 |
| Si | 0.40 | 0.40 | 0.45 | 0.45 |
| Mn | 1.20 | 1.20 | 1.40 | 1.30 |
| P | 0.025 | 0.025 | 0.025 | 0.025 |
| S | 0.015 | 0.015 | 0.015 | 0.015 |
| V / Nb / Ti | 0.06 / 0.05 / 0.04 | 0.06 / 0.05 / 0.04 | 0.05 / 0.05 / 0.04 | 0.05 / 0.05 / 0.04 |
| CEIIW / CEPcm | 0.43 / 0.25 | 0.43 / 0.25 | 0.43 / 0.25 | 0.43 / 0.25 |
| Availability | Seamless or welded | Welded only | ||
R is as-rolled, N is normalised, Q is quenched and tempered, M is thermomechanically rolled. X42M exists only in the welded column of Table 6; there is no seamless X42M. Carbon equivalent limits apply above 0.12% carbon as CEIIW and at or below 0.12% as CEPcm.
Now the arithmetic. Take the element limits at their maximums and calculate CEIIW as C + Mn/6, ignoring residuals and vanadium, which only push it higher.
| Condition | C | Mn | CEIIW | Against the 0.43 ceiling |
|---|---|---|---|---|
| PSL1 welded, at limit | 0.26 | 1.30 | 0.477 | No ceiling applies at PSL1 |
| X42R / X42N, at limit | 0.24 | 1.20 | 0.440 | Over by 0.010 |
| X42M, at limit | 0.22 | 1.30 | 0.437 | Over by 0.007 |
| X42Q, at limit | 0.18 | 1.40 | 0.413 | Under by 0.017 |
So at X42 the element limits and the carbon equivalent ceiling cannot both be taken at face value. A mill that runs X42R at 0.24 carbon and 1.20 manganese fails its own carbon equivalent limit by one hundredth of a percent, and a ladle analysis at 0.24/1.20 is not an absurd target - it is what a mill reaching for yield would aim at. The certificate that arrives will show something nearer 0.21 carbon and 1.15 manganese, and the buyer who expected the table maxima will read that as a leaner heat than ordered.
There is a second effect worth understanding, because it is counter-intuitive. The manganese credit lets the mill trade carbon for manganese: 0.01% less carbon buys 0.05% more manganese. On carbon equivalent that trade is almost exactly neutral - 0.01 off carbon removes 0.010, and 0.05 of manganese adds 0.008. Work it through and the ceiling only clears at the bottom of the walk:
| C | Mn allowed | CEIIW |
|---|---|---|
| 0.24 | 1.20 | 0.440 |
| 0.22 | 1.30 | 0.437 |
| 0.20 | 1.40 | 0.433 |
| 0.18 | 1.50 | 0.430 |
To hold 0.43 while taking the manganese credit in full, carbon has to come down to 0.18% and no further credit is left. That is precisely the X42Q carbon limit, which is not a coincidence - the Q grade's chemistry is drawn where the credit and the ceiling meet. It also explains why X42Q is the grade mills quote when a specification calls for a carbon equivalent without naming a delivery condition, and why a quotation for X42R at an unusually good price deserves a question about which of the two numbers it is holding.
Strength: Same Floor, Different Ceiling
| Property | PSL1 | PSL2 |
|---|---|---|
| Yield strength, MPa | 290 min | 290–495 |
| Tensile strength, MPa | 415 min | 415–655 |
| Weld seam tensile, MPa | 415 min | 415 min |
| Yield to tensile ratio | Not specified | ≤ 0.93 above 323.9 mm OD |
| Elongation | Per formula | Per formula, same equation |
Both levels start at 290 MPa. PSL2 adds a ceiling of 495 MPa, which is 205 MPa above the floor, and a tensile ceiling of 655 MPa. Note that 655, not 760: the higher tensile ceiling in Table 7 belongs to grades above X46, and X42 does not get it. An X42 heat that pulls 700 MPa tensile is not a better X42, it is a non-conforming one, and the reason is that a pipe 69% stronger in tension than its design basis has given up the ductility the design assumed.
The 0.93 ratio applies only above 323.9 mm outside diameter, which is worth knowing because a 12 inch order sits just under that line and a 14 inch order just over it. Below the line, the ratio is not a requirement and no value will appear on the certificate.
Elongation is not a fixed number in API 5L; it is calculated from the test piece and the specified tensile strength.
Af = 1 940 × Axc0.2 / U0.9
For X42, with U at 415 MPa, that gives 23% for a 12.7 mm round bar, 20% for a 6.4 mm bar, and 29% for a full-section strip. The 21% figure that appears on a great many X42 pages is not one of these numbers and does not come from the equation; it is a rounding that has been copied from page to page. Quote the formula, or quote the value that matches the test piece in your specification, and the two will agree.
Toughness: What PSL2 Tests, and What It Does Not
PSL1 requires no impact testing at all. That is not a loophole; it is the level's design intent, and a PSL1 X42 line in dry gas at low pressure has no need of it. PSL2 makes Charpy mandatory for every test unit, at 0 °C unless a lower temperature is agreed.
| Test location | Requirement at X42 |
|---|---|
| Pipe body, OD up to 762 mm | 27 J average, full-size specimen |
| Pipe body, OD above 762 mm | 40 J average, full-size specimen |
| Seam weld | 27 J average of three, at 0 °C |
| Heat-affected zone | 27 J average of three, on SAWL and SAWH; not sampled on HFW |
The HFW exemption is practical rather than metallurgical: the HAZ of a high-frequency weld is too narrow to sample accurately with a Charpy specimen. It does not mean the zone is tougher - it means the test cannot see it, and the process control has to carry the argument instead.
Two things this table does not say, and both are commonly assumed. It does not require a drop-weight tear test. DWTT belongs to the large-diameter, high-grade gas transmission world where crack arrest governs the design; at X42 in the sizes this grade is bought, the fracture argument is carried by Charpy upper-shelf energy and by the seam being sound. If a project specification asks for DWTT on X42, that is a purchaser requirement and it should be priced as one. And it does not require a hardness survey. Hardness limits at 250 HV10 come from Annex H, which applies only when the pipe is ordered for sour service with the S suffix.
X42 Against Grade B: 15% of the Steel, and Where It Disappears
Grade B and X42 have the same minimum tensile strength, 415 MPa. They differ only in minimum yield, 245 against 290 MPa, and because wall thickness under pressure scales with yield, that difference converts directly into steel.
| Case | X42 wall | X42 weight | Grade B wall | Grade B weight | Saving |
|---|---|---|---|---|---|
| 323.9 mm at 6.3 MPa | 4.89 mm | 38.4 kg/m | 5.78 mm | 45.4 kg/m | 15.3% |
| 610 mm at 7.0 MPa | 10.23 mm | 151.2 kg/m | 12.10 mm | 178.5 kg/m | 15.3% |
| 762 mm at 7.0 MPa | 12.77 mm | 236.0 kg/m | 15.12 mm | 278.5 kg/m | 15.3% |
Barlow, P = 2St/D, with design factor 0.72 and no corrosion allowance. The saving is constant because 245/290 is constant: 15.5% less wall, 15.3% less weight once the wall is subtracted from the diameter. On a 300 km line of 610 mm pipe that is roughly 8,000 tonnes.
That is the case for X42, and it is a good one - but it only exists where pressure sets the wall. In distribution it usually does not. Run the same arithmetic at the pressures a distribution main actually sees and the result stops being useful.
A 4 inch line at 4 bar needs 0.11 mm of wall to hold the hoop stress at 290 MPa with a design factor of 0.72. It is bought at 6.02 mm, Schedule 40, which is fifty-five times thicker. The wall is not there for pressure. It is there to survive being unloaded, strung, bent, welded and tapped, to carry a corrosion allowance on wet gas, and to leave metal under the thread or the service tee. Swapping Grade B for X42 in that pipe saves nothing at all, because both grades are ordered at the same schedule.
This is the honest version of the X42 story. It is a transmission and medium-pressure grade. Below about 6 inch and below about 7 bar, the grade choice is a purchasing habit rather than an engineering decision, and the money is better spent on coating, on the seam, or on the fittings.
What Comes Off Each Line
ERW and HFW
Coil is slit to width, the edges are trimmed and scarfed, and the strip is formed through a series of rolls into a cylinder that is still open at the seam. Two squeeze rolls press the edges together while current passes through them and the resistance at the contact face does the melting. The flash is scarfed off outside and, on most lines, inside as well. The seam then passes an in-line normalising inductor before the pipe is sized and cut.
Three defects belong to this process and no other. A cold weld is a seam that closed without reaching welding temperature - it looks continuous, it passes a flattening test more often than it should, and it separates under pressure. A penetrator is a short, hard, unbonded segment inside the seam, historically the signature failure of low-frequency machines. A hook crack opens at the fusion line where the strip edge has been deformed by the squeeze rolls, and it runs into the wall rather than along the seam. All three are longitudinal, all three are found by ultrasonic inspection with the beam angled across the seam, and none is found by radiography in a thin wall.
LSAW
Plate is crimped at the edges, pressed into a J or a U, closed into an O, and welded with one pass inside and one outside, each usually multi-wire. The pipe is then cold expanded to a sizing ratio between 0.003 and 0.015 - the clause that gives LSAW its roundness and its accurate circumference. Expansion also relieves the welding stress and equalises yield around the circumference, which is why an LSAW pipe measures better at the ends than an unexpanded one.
Its characteristic defect is lack of sidewall fusion at the root, where the inside pass has not reached the plate faces. It is planar, it is oriented along the seam, and it is exactly the defect an angled shear-wave scan is for. One clause worth carrying into the order: coil and plate end welds may not be present in finished longitudinal seam pipe at all. In helical pipe they may, provided the junction with the spiral sits at least 300 mm from the pipe ends.
SSAW
Coil is fed into the forming head at an angle, and the pipe is in effect a rolled strip whose width becomes the circumference divided by the cosine of that angle. Weld length per metre of pipe is the circumference divided by the strip width, so a 1219 mm pipe from 1500 mm coil carries 2.55 m of seam in every metre - 30.6 m in a 12 m joint. Both sides are welded with submerged arc, and the spiral is continuous from end to end.
Alignment is the sensitive variable. A mismatch at the spiral edge shows up as a step in the seam that the inside pass has to bridge, and the resulting defect is again planar. The T where the spiral meets a girth weld is the least friendly geometry in the pipe for any volumetric inspection, and on a line that will be inspected by automatic ultrasonic testing this is the location that generates the indications requiring evaluation.
Inspection, and What to Add
The standard's baseline is a hydrostatic test on every joint, plus non-destructive inspection of the seam. At PSL1 that inspection is required only when the purchaser specifies it. At PSL2 it is mandatory, and the acceptance criteria are tighter. Hydrostatic test pressure is set by the mill within the standard, typically between 60% and 90% of the specified minimum yield strength, held for at least five seconds up to 457 mm and ten seconds above it.
Four additions are worth the money on a welded X42 order, and each addresses something the standard leaves open:
Full-length seam ultrasonic inspection with a phased array, recorded. Not a spot check at the ends. The defects that matter in an ERW seam are short and they are not distributed evenly along the joint.
Flattening test frequency. The standard requires flattening on ERW pipe, and it is the one mechanical test that loads the seam the way site handling will. Ask how many joints per lot are tested, not whether the test exists.
Weld tensile and transverse bend on the seam. These show whether the weld is undermatching the body, which on a lean X42 heat is a real possibility.
Hardness traverse across the seam and heat-affected zone. Only relevant to sour or wet service, but if the service is sour, this is the test that reveals whether the seam treatment actually did what it claimed.
Measurement of the pipe itself is worth a mention because it is where cheap pipe diverges first. End squareness, circumference at both ends, and wall thickness at the seam are the three figures that decide whether the joint will fit up in the ditch. A pipe that is 1.5 mm out of round at the end will cost more in welding time on a spread than it saved per tonne.
Coating, Ends and Handling
Coating choice follows the soil and the service, not the grade. Three-layer polyethylene for buried transmission and distribution mains, fusion bonded epoxy where the operating temperature is high or the pipe will be handled roughly, three-layer polypropylene above 70 °C, coal tar epoxy for immersed or aggressive ground, and black varnish where the pipe is going into a warehouse rather than a trench. Internal flow coating is worth considering on water and slurry lines at X42, because the grade is often chosen for exactly those services and the internal friction loss is a permanent operating cost.
Ends are plain, bevelled, or threaded and coupled. For ERW pipe below 2 inch, threaded and coupled is still normal in distribution, and the wall under the thread is the governing thickness - a point that catches out buyers who specify a wall from a pressure calculation and forget the thread depth. For bevelled ends, the bevel angle and root face should match the welding procedure the contractor will actually use, which is not always 30° and 1.6 mm.
Where X42 Welded Pipe Is Used
Gas distribution mains and services - the largest single use of the grade in tonnage terms, at pressures from a few bar to 20 bar.
Gathering lines - wellhead to processing, often wet and often small diameter, where PSL2 and a sour specification may be layered on.
Water transmission and distribution - potable and raw water mains, where X42 is chosen for handling strength rather than pressure.
Slurry and tailings lines - mining duty, usually with a wear allowance added to the wall.
Water injection and disposal lines - oilfield produced water, frequently with internal coating or lining.
Fire mains and plant piping - where the pipe is bought to a line pipe standard for availability rather than for pressure.
Low and medium pressure process lines - steam, condensate and utility headers in plants that standardise on line pipe.
One caution on that list. X42 is often reached for on piling and structural work because it is cheap and available, and a line pipe certificate does not satisfy a piling specification. If the pipe is going into the ground to carry load rather than fluid, the standard to order against is ASTM A252, which is written around driving and splice strength and does not require a hydrostatic test. The two are not interchangeable, and the difference shows up at the first inspection of the foundation.
The Ordering Lines
Six lines carry almost all of the risk on a welded X42 order. Every one of them is a place where the standard offers a choice and silence means the mill chooses.
Pipe type. Type E, W or S - or in plain words, ERW, LSAW or SSAW. "Welded" alone does not specify a product.
PSL. PSL1 or PSL2. This decides whether the seam treatment has an alternative, whether Charpy is run, and whether the certificate exists by default.
Delivery condition where PSL2 is called for: R, N, Q or M, written into the grade as X42Q and not left to the mill.
Seam heat treatment where PSL1 is called for and the service is more than utility: name it as normalising simulated over the full seam and HAZ, and require it to be recorded.
Inspection coverage and standard. Which NDT method, over what length, to which acceptance level, and whether records travel with the pipe.
Certificate. EN 10204 3.1 as a minimum. At PSL1, the certificate is issued only if the order asks for it, and traceability is required only until the tests are passed - which is why PSL1 pipe often arrives with paperwork that cannot be tied back to the joint in your hand.
Two further traps are worth knowing. Schedule is not wall thickness. A SCH 40 pipe is a nominal wall with a tolerance, and the tolerance for welded pipe is not the same as for seamless; if the design needs a minimum wall, order a minimum wall and not a schedule. And "API 5L X42" written without a year refers to whichever edition the mill works to - the 45th and 46th editions differ in detail, and a specification written against one of them should say so.
Test and inspection



Send The Line Schedule And We Will Price It Properly
Give us the diameter, wall or schedule, total metres, service and design pressure, the PSL you need or the one you think you need, coating and end finish, and the destination port. We will come back with the route we would use at that size - ERW, LSAW or spiral - the seam treatment and inspection coverage that go with it, and a price that can be compared line for line with any other offer you are holding.
FAQ
What does X42 mean, and is it the same as L290?
X42 is API 5L's designation for a minimum yield strength of 42,100 psi, which is 290 MPa. ISO 3183, which is technically identical to API 5L, writes the same grade as L290. GB/T 9711 uses L290 as well. The number is a minimum yield, not a tensile strength and not a wall thickness - the minimum tensile at X42 is 415 MPa, the same as Grade B.
Is X42 welded pipe as good as seamless?
For the services X42 is used in, yes, provided the order specifies which seam treatment and which inspection apply. A welded seam is a controlled, tested, inspectable feature, and modern HFW seams in PSL2 pipe are held to a normalising treatment and full-length inspection that seamless pipe never has to demonstrate. The honest qualification is that the quality of a welded seam varies more between suppliers than the quality of a seamless wall does, because the process has more variables - which is a reason to specify, not a reason to avoid.
Does PSL2 make the pipe stronger?
No. The minimum yield is 290 MPa at both levels. PSL2 adds an upper limit of 495 MPa, mandatory Charpy testing, a carbon equivalent ceiling, 100 kHz minimum welding frequency, mandatory seam inspection and full traceability. What you buy with PSL2 is consistency and evidence, not strength - and a pipe that comes in at 480 MPa yield against a 290 MPa design basis is not a bonus, it is a heat that used more alloy than it needed.
Can I order X42M?
Only as welded pipe. X42M is thermomechanically rolled and appears in the welded column of API 5L Table 6; the seamless column has no M grade. If a quotation offers seamless X42M, either the grade or the pipe type is wrong. X42R, X42N and X42Q are available in both seamless and welded.
Why is one X42 quotation so much cheaper than another?
Usually because it is a different product. The common differences are PSL1 instead of PSL2, no seam inspection beyond the hydrostatic test, no Charpy, a certificate that exists as a test report rather than a 3.1 inspection certificate, and a seam treatment that used the alternative permitted at X42. Any one of those is legitimate if it matches the service; all four together are what a low quotation for "API 5L X42 ERW" usually means. Ask for the four items in writing and the gap will explain itself.
What is the largest diameter available in welded X42?
ERW stops at about 609.6 mm (24 in) and a few mills quote 26 in. LSAW runs to roughly 1524 mm (60 in). SSAW goes to 2540 mm (100 in) and beyond on wide coil. Above 1524 mm, spiral is effectively the only route, and at that point the wall is limited by coil thickness rather than by the grade.
Can X42 welded pipe be used in sour service?
It can, and the qualification is not simply a grade choice. Sour service requires the S suffix on the delivery condition - X42QS or X42MS - which brings the pipe under Annex H, with lower sulphur, a hardness ceiling of 250 HV10, and HIC and SSC testing. A standard X42 order does not meet Annex H however good the steel is, and neither does a certificate that says "NACE" without naming the test and the acceptance criteria.
Hot Tags: welded api 5l x42 steel pipe, China welded api 5l x42 steel pipe manufacturers, suppliers, factory, China Q345 Welded Steel Tube, SY T5037 2018, spiral steel pipe, SY T5037 Steel Pipe, SY T 5040 Welded Steel Pipe, A335 P1 Welded Carbon Steel Tube